How to repair tension marks on precision piston rods

If the precision piston rod is pulled during operation and not treated in a timely manner, it can affect the use of the product in mild cases, and in severe cases, make the hydraulic cylinder unable to work. So how do we fix it? Local grinding and polishing methods are used to repair lighter pull marks; For heavier pull marks, welding repair and manual grinding are used to repair them.
Formation of pull marks: After disassembling the gas-liquid booster cylinder, it was found that a precision piston rod was severely pulled, with 6 pull marks arranged side by side. The main reason for the pulling injury is that after the dust ring becomes brittle and falls off in a block like manner, it not only loses its dust prevention effect, but also accumulates a lot of dust and impurities in the expansion joint, causing the piston rod to grind hard with impurities, resulting in pulling injury. The scars then scratch the rubber sealing components at the cylinder port, causing serious leakage of the hydraulic cylinder.
Repair requirements: The filler and base material should be combined stably and smoothly; The seasoning must be easy to use and easy to manually process; Manual processing should ensure that the diameter error of the precision piston rod is less than 0.06mm. After analysis, it was decided to use J422 welding rod as the filler. Because acidic welding rods are not sensitive to rust, oil stains, and moisture, and are not prone to generating hydrogenated pores; Good craftsmanship and easy operation; Beautiful welding seam formation; The material has moderate hardness and is easy to process by hand; Stable arc, large melting depth, and stable bonding with the base material.
Repair process:
1. Clean the area to be welded first, and then surround the pull marks with damp mud.
2. Select a welding rod with a diameter of 2.5mm, adjust the current of the welding machine to 120A, and use the straight line welding method to smoothly weld.
3. After all welding is completed, clean the mud and slag, and use a rough file to file along the circumference of the precision piston rod, leaving a machining allowance of 0.1-0.2mm.
4. A cylinder with an outer diameter of 185mm, an inner diameter of 125mm, and a length of 150mm is used as a model (the outer diameter of the piston rod is 125mm). It is sawn along the axis, with one being a rough model and the other being a precision model.
5. Apply a thin layer of red ink on the inner wall of the rough mold, and then rub the rough mold tightly against the area to be repaired along the axis several times. Then, use a fine file to remove the heavier red ink on the product. Repeat the filing process and leave a machining allowance of 0.04-0.07mm.
6. Then use a 320 mesh sand strip dipped in kerosene and fine mold to grind the product to the specified size.
7. Afterwards, dip the back of the sandcloth in kerosene for manual polishing. After measurement, the significant error is only 0.03mm.

主站蜘蛛池模板: 欧美亚洲图区| 久久综合狠狠综合狠狠| 亚洲国产成人久久综合一| 亚洲一区二区在线| 97影院午夜午夜伦不卡| 黄色1级视频| 日本成人精品| 天天爽夜夜爽人人爽免费| 亚洲综合视频在线| 国产呦在线观看视频| 欧洲精品码一区二区三区免费看 | 绝色村妇的泛滥春情| 日本视频www色| 天天视频国产精品| 国产免费人人看大香伊| 青青青手机在线视频| 四虎永久在线精品国产| 亚洲一二三四区| 欧美一级爽快片淫片高清在线观看| 日日夜夜免费视频| 亚洲福利一区二区三区| 免费a在线看| 色综合久久88中文字幕| 亚洲专区一区| 拍拍拍交性免费视频| 污夜影院| 成人国内精品久久久久影院| 欧美猛操| 天天好比网| 成年女人免费看一级人体片| 色www视频永久免费| 亚洲国产日韩欧美在线as乱码| 国产精品久久久久国产精品三级| 人人干人人上| 亚洲 国产精品 日韩| 国产亚洲精品aa在线看| 日韩欧美精品综合久久| 亚洲一区二区三区不卡视频| 青青草99热久久| 亚洲欧美日韩三级| 免费看片你懂的|